Posted in Sign & Display media for HP Latex printers by Mary Hester Mon Sep 20 2021 13:55:05 GMT+0000 (Coordinated Universal Time)·1·Viewed 484 times

I am running an HP335Latex. I'm running Nekoosa 9RTape) OM 14Mil Synaps which ran easily on my old 310 printer, but using the same profile warps when it goes through the heaters on my new 335. I'm running it as a 12 pass, 207degree heat, 100% saturation. What can I do to lower the heaters so that it will still cure correctly, but not warp the material. Can I submit a photo, so you can see what it's doing?
Sep 20, 2021

Magical solution seems to be 20 pass, 189 heat, 90% saturation. It takes longer to print, but at least it lays flat now.

  